Package Strength Testing

Package strength testing measures how much force the seals of a pack and the case around it hold before they open or crush. On a form-fill-seal, sachet or pouch line that means three tests: a peel test on a strip cut through the seal, a burst test on the whole sealed pack, and a compression test on the closed case behind the case packer.

Strength and integrity are two different questions. A seal can pull at full strength and still carry a channel leak, and a pack can be leak-tight with a seal that opens in the customer’s hand.

Which Tests Measure Package Strength

Three tests, each loading a different part of the pack: seal peel pulls a strip cut through one seal, burst pressurises the whole sealed pack until a seal gives, and box compression presses the closed case until it buckles. Drop, vibration and the full distribution sequence load the whole shipper the way transit will; they are covered under packaging integrity testing, and this article does not repeat them.

Seal Peel Test (ASTM F88)

Cut a strip 25 mm (1 in) wide across the seal, clamp the two free tails in a tensile tester and pull them apart at a constant rate — 200–250 mm/min in the published studies that run the method. The result is the peak force per unit width plus the failure mode: whether the seal peeled, the film tore beside it, or the layers delaminated.

The standard gives three ways to hold the tails: unsupported, hand-supported at 90°, or supported at 180°. Pick one and keep it for every sample; readings taken with different techniques do not compare.

A spec carries a lower limit, which guarantees closure, and on peelable packs an upper limit, which keeps the pack openable. On the line, sample every seal the machine makes — back or fin seal, top and bottom cross-seals — and on a multi-lane sachet or stick pack machine every lane.

Burst Test (ASTM F1140 / F2054)

The pack is inflated through a needle at a controlled rate until a seal opens, and the peak pressure is the result. For a pouch sealed around its perimeter — every sachet, stick pack and pre-made pouch — use the restrained method, F2054: the pack inflates between two plates, so the stress runs evenly along the seal perimeter and the weakest point is the one that opens. Unrestrained F1140 lets the pack balloon and can miss the weakest seal.

The value compares only like with like. Pack size, seal type, inflation rate and plate gap all move the number, so a burst figure from a different pack size, or from the film supplier’s lab, says nothing about yours. Nor does it convert to F88: the standards state that the two do not necessarily correlate, so peel and burst are two separate trends.

Box Compression Test (BCT) and ECT

The case packer and palletizer end needs one number: the load the closed, filled case takes before it buckles. BCT under ASTM D642 / TAPPI T 804 puts the case between two platens closing at 12.7 mm/min (0.5 in/min) and records the peak load, after the case has been conditioned at 23 °C and 50 % RH. ECT is the board supplier’s number, measured on a short column of board, and it feeds the estimate behind the online calculators:

BCT = 5.87 × ECT × √(t × Z)

with BCT in lb, ECT in lb/in, and board caliper t and box perimeter Z in inches. Use it to size the board before the cases exist. In a published test on plain RSC cases the simplified form was off by up to 18 %, and it does not hold for cases with hand holes or cutouts, so run BCT on the real filled case once you have it.

For a safe stack, divide the tested BCT by a factor of about 3 for the allowable load on the bottom case — the value unit-load design studies adopt to meet ISTA 3E — and more under long storage or high humidity. Then check the pattern the palletizing robot lays: a case hanging over the pallet edge loses between 0 and 40 % of its tested compression strength in Virginia Tech measurements, depending on how far it overhangs.

What a Low Result Points to on the Machine

A low or scattered seal-strength result is a sealing-parameter problem before it is a film problem: jaw temperature, dwell, jaw pressure, the condition of the jaw faces and their PTFE cover, or a reel that seals differently from the last one. Do not expect the film supplier’s F88 sheet to be your target either: ASTM’s own heat-seal practice, F2029, calls a bench-sealer curve a starting point for the production setting.

Where the reading is low points to the cause:

  • One seal position low: that jaw. On a VFFS with the back seal fine and the bottom seal low, look at the cross-seal jaws — alignment, a worn face, pressure uneven across the width.
  • One lane low: that lane’s heater zone, jaw face or film tension on a multi-lane sachet or stick-pack machine.
  • Everything drifting down over a shift: temperature control or the film reel. A heater losing control moves every seal at once; a drop that starts at a reel change points to the film.

A seal that passes F88 cold but opens on the line at speed is a different limit: hot tack, the strength of the seal in the instant after the jaw opens, while the product drop is already loading it. That is set by the film’s sealant layer, covered in film sealant layers and VFFS speed.

How Many Packs to Test, and When

Pull several strips from each seal position and each lane at every event that can move the seal — start-up, changeover, a film reel change, a jaw change — and once per shift in between. Published studies running F88 pull four to ten strips per condition; several per position is enough to show whether one jaw is scattering.

Let the pack cool to room temperature before cutting the strip, so every sample is tested in the same state.

Keep the results as a per-jaw and per-lane trend. A batch average across all lanes hides a drifting lane until it fails.

    Comments are closed

    Soontact provides complete packaging solutions for manufacturers worldwide. Contact our packaging engineers to discuss your specific products, production volumes, and packaging material requirements.

    We offer machine demonstrations, application testing, and detailed proposals that address your particular operational needs.